IXPE foam

A foam spacer between two cells looks like the simplest part in the module. It has no connector, no coating and no orientation, and on the drawing it is often a rectangle with three lines of text: material, thickness, density. First article is where the simplicity ends. The quality engineer has a batch certificate that lists a compression set value, a drawing that names a thickness, and a module that compresses the part by some amount nobody wrote down. Three questions follow: what force does this part push back with, what thickness will it keep, and which of those numbers is an acceptance criterion?

The honest answer is that the material sheet answers part of the second question and neither of the others. This article separates the quantities, shows the conditions attached to each published number, and sets out a test plan that assigns every measurement to the party able to make it. It is written for the module maker and the foam converter who have to sign the same drawing.

1. A spacer is a spring, a memory and a piece of sheet

Three descriptions of the same rectangle, used for three different decisions.

As a spring, it has a force at a deflection. The module cares about this because the spacer sits in the load path of the cell stack, and the force it adds at installed compression is part of the stack's equilibrium.

As a memory, it has a compression set: the fraction of a defined squeeze it does not recover. The drawing cares about this because the gap after a year is not the gap at assembly.

As a piece of sheet, it has a thickness and a tolerance. Purchasing cares about this because the part is cut from a sheet whose thickness varies within a band, and the cut profile has its own tolerance.

The trap is that all three get written as percentages or millimetres on one line, and then read as if they were one property. They are measured by three different parties on three different objects: the module fixture, the material laboratory, and the converter's inspection bench.

2. Force at installed compression is a stack measurement

No catalogue can give the force a die-cut spacer develops in a specific module, and a supplier who offers one should be asked how it was measured. The force depends on the expansion ratio, the free thickness, the installed compression, the loaded area, the shape of the part, whether it is laminated, and the rate at which it is compressed. A curve measured on a 10 mm sheet at one ratio does not transfer to a 2 mm die-cut ring with an adhesive backing.

Two measurement conditions decide whether two force numbers can be compared at all: the rate of compression and the preload. A hand press, a testing machine closing at a constant rate and a module fixture that closes in one step will not produce the same curve. Write the rate and the fixture into the requirement, or the two parties will report different forces for the same part and both be right.

What can be done instead is straightforward. The module maker compresses the actual stack — cells, spacers, end plates, fixtures — and records force against deflection. The foam supplier holds the inputs constant: ratio, density band, thickness, and set behaviour at the stated condition. The two records then meet on the drawing as a force window at a stated compression, with the test owner named.

One design point is worth stating plainly because it is often inverted. In a clamped stack, the clamp load is set by the structure, not by the pad. Fitting a softer foam does not reduce the load on the cell; it changes how much of the stack tolerance the pad absorbs and where the compression ends up. If cell stress is the concern, it is answered by the clamping design and by cell data. A softer spacer is not a substitute for either.

3. What the set number reports

Compression set is measured by squeezing a specimen to a fixed ratio, holding it at a fixed temperature for a fixed time, releasing it, and measuring the thickness that does not come back. Our sheets report GB/T 6669 at 23±2 °C for 22 hours. The values are listed by expansion ratio because the material changes across the range.

Compression set by expansion ratio (GB/T 6669, 23±2 °C, 22 h)
Grade3×5×8×10×15×20×25×30×35×40×
XPE≤2%≤2%≤3%≤5%≤7%≤8%≤10%≤10%≤11%≤11%
IXPE≤2%≤2%≤3%≤5%≤7%≤8%≤9%≤10%≤11%≤11%

Read across the row, not down a column. At 3× the allowance is ≤2%; at 35× and 40× it is ≤11%. Both are XPE or IXPE; they are not interchangeable parts. A specification that quotes one set value for "XPE foam" without the ratio has thrown away the part of the number that changes.

Two limits belong to this test. It is run on a specimen, not on the die-cut part, so edges, adhesive and lamination are not represented. And it is a single squeeze over 22 hours, not a service-life test; it says what the material remembers after one defined event, not what it will remember after a year of thermal cycling.

4. Two conditions that travel with every set value

The test ratio. The standard defines how far the specimen is compressed, and the test report carries the value. Two suppliers can both say "compression set ≤5%" and mean different things if one tested at 25% compression and the other at 50%. Ask for the ratio, the specimen thickness and the test standard on the certificate.

The temperature and time. 23 °C and 22 hours is a laboratory condition. A battery module in service is frequently warmer, and the direction of the effect is not in dispute: more heat and more time generally produce more set. The size of the effect at a given service temperature is not on our sheet, and we will not invent one. The 70 °C data we publish is a dimensional change test (GB/T 8811), which measures shrinkage of an unrestrained sheet. It is not a set value and cannot be substituted for one.

5. "Rebound" needs five parameters before it is a criterion

Drawings often ask for "good rebound" or "high resilience". The word points at a real behaviour, but it can mean at least three different measurements: height recovery after one compression, energy return in a dynamic cycle, or the absence of permanent deformation after storage. Each has its own test and its own answer.

We publish no rebound percentage, no hysteresis and no dynamic stiffness. What we can do is agree a part-level test. Five parameters make the word measurable: the compression as a percentage of free thickness, the number of cycles, the temperature, the recovery time before measurement, and the acceptance tolerance. With those five written down, "rebound" becomes a check an inspector can run. Without them, it is a preference that cannot fail.

Choose the test by the duty. A spacer assembled once and never opened is governed by set, not by cycling. A spacer that is opened for service or reworked is governed by cycling, and the test should run on the part, with the real edge conditions, not be inferred from a material sheet.

6. Three thicknesses, three owners

Free thickness is the nominal on the drawing. Installed thickness is what remains after the stack closes. Tolerance is the permitted deviation of the cut part, which is not the same as the permitted deviation of the sheet.

Supply ranges matter here. XPE is supplied from 3 mm in a single layer; IXPE from 0.1 mm. Multi-layer laminated sheet runs 15–200 mm for both. IXPP, where temperature points to it, is 1–6 mm in a single layer and 6–100 mm laminated. A 2 mm XPE spacer is therefore not a single-layer part; it is either IXPE or a laminated construction, and the drawing should say which.

The tolerance chain is where spacers get into trouble. Cell thickness, spacer thickness, tray flatness and end-plate flatness all contribute. The pad has to absorb the sum while staying inside the compression range where its set data still applies. If the sum is too large, the answer is a stack redesign or a hard shim, not a softer grade. And converting tolerance is a separate line: die-cutting and CNC routing have dimensional limits of their own, so a 10 mm sheet cut to a profile is not automatically a 10.00 mm part.

Laminated thickness deserves its own note. A 30 mm spacer built from layers is not the same part as a 15 mm single sheet, even at the same density: the interfaces between layers are planes where shear can start, and a compression set measured on a solid specimen does not describe them. If the design needs the thickness, ask for the layer construction and inspect the bond line at first article.

7. A first-article plan that names the owner

First-article measurements for one spacer
MeasurementMethodWho produces itWhat is recorded
Free thickness at defined pointsMicrometer, points agreed on the drawingConverterValues and tolerance band
Compression setGB/T 6669, 23±2 °C, 22 hMaterial supplier, batch certificateValue, test ratio, specimen thickness
Dimensional change at 70 °CGB/T 8811, 70±2 °C, 22 hMaterial supplierCross and machine direction values
Force at installed compressionCompress the actual stackModule makerForce window at the stated compression
Appearance and edge qualityVisual against an agreed sampleConverterBurrs, lamination gaps, adhesive coverage

Two absences are deliberate. There is no force value from the foam supplier, because no catalogue curve describes this part in this stack. And there is no life prediction, because the published tests are single events at stated conditions. A first-article report that fills those gaps with estimates is less useful than one that leaves them open and assigns them.

8. The number we will not publish, and why that is useful

Service temperature is the gap that matters most in a battery module. Our set data is at 23 °C; the part may sit well above that for most of its life. The effect of temperature on set is real and directionally known, but its magnitude for a given grade and history is not something we publish. A supplier who quotes "set at 60 °C: 8%" from a catalogue has either tested it or made it up; ask which.

The constructive answer is a qualification test on the part at the service temperature, with the installed compression and a duration taken from the module validation plan. That test belongs in the module qualification, not on the foam datasheet, and it should be run before the drawing is frozen rather than after the first field return.

The dimensional change data we do publish runs to 4% across and 6% along the sheet at 15× and below, and to 6% and 8% at 20× and above (GB/T 8811, 70±2 °C, 22 h). Read it as a shrinkage allowance for a free sheet, not as a recovery figure.

9. What goes on the drawing, and where the spacer stops

A drawing that can be accepted without argument carries these lines:

  • material and expansion ratio, or a density band;
  • free thickness with tolerance, and the installed compression or installed gap;
  • force window at installed compression, and who measures it;
  • compression set value, test standard and test ratio;
  • service temperature range;
  • part dimensions and converting tolerance, stated separately from sheet tolerance;
  • adhesive, if any, and its temperature limit;
  • packaging and quantity.

And these are the things the spacer does not do. It does not manage cell swelling by itself; it does not replace the clamp design; it does not guarantee a force over life; it is not a fire barrier; it does not carry a dielectric strength figure; and it does not define the gap without the rest of the tolerance chain.

To quote a spacer, send the drawing and the stack details: free thickness, installed compression, service temperature and quantity. Bofeng Foam has manufactured cross-linked polyolefin foam since 2011, with five production lines and 5,000 tonnes per year at a 10,000 m² plant. Standard material starts at 1,000 m²; custom parts are quoted from the drawing. A4 samples are free including freight, and lead time is typically 15–20 days. The material pages for IXPE and XPE carry the full property tables, and the battery pack selection guide covers the thermal and flame questions that sit next to this one, and the energy storage battery foam application page shows the interfaces this spacer sits between.